In vitro degradation testing for scaffolds and implants
A scaffold degradation test should match the device: the sterilized, finished form at its real porosity and print pattern, with mass, molecular weight and mechanics read together. ASTM F1635 and ISO 13781 set out the hydrolytic method for implant polymers. The form matters before the run starts: in one study, gamma irradiation cut a PLGA scaffold’s molecular weight by about half.
Where do ASTM F1635 and ISO 13781 apply most directly?
Both standards were written for implants, so a scaffold or a degradable implant is their home ground. ASTM F1635’s public scope covers hydrolytically degradable polymers for surgical implants, as virgin resin and as fabricated forms, including sterilized implants and purpose-made specimens. It adds that results from a resin or a semi-finished form aren’t sufficient to predict how the final sterilized implant degrades.
ISO 13781’s scope covers polylactide homopolymers, copolymers and blends, in bulk or processed form, up to finished, packaged and sterilized implants. The degradation testing guide covers what F1635 asks you to measure, its limits on loading, and how size, flow and temperature move the rate. A collagen, chitosan or hyaluronic acid scaffold sits outside F1635, which excludes polymers that degrade mainly by other mechanisms; hydrolytic versus enzymatic degradation covers that test.
How does sterilization change the result?
Sterilization can change the polymer before the test begins, so test the sterilized form. F1635’s public page says sterilization should be expected to change molar mass, structure or both. To represent in vivo performance, specimens are packaged and sterilized like the final device, with non-sterilized ones allowed for comparison.
Holy and colleagues compared three methods on a porous PLGA scaffold, against ethanol disinfection as a control:
- Ethylene oxide: the scaffolds shrank to 60% of their starting volume.
- Gamma irradiation: weight-average molecular weight fell by about half, and these samples changed most in shape and volume over 8 weeks of degradation.
- Argon plasma: the authors rated it best, for the least deformation.
Over the 8 weeks, ethylene oxide, plasma and ethanol samples followed similar molecular weight and mass curves. Gamma was the method that changed the polymer itself, so its effect shows in the degradation data. Sterilizing every test sample the way the device will be sterilized costs a run through the process, and skipping it can leave you measuring a different polymer.
How do porosity and print pattern change the result?
Porosity moves the rate, and print pattern moves the mechanics. Agrawal and colleagues degraded PLGA scaffolds of different porosity in PBS at 37 °C for up to 6 weeks: the lower the porosity and permeability, the faster they degraded. The authors suggest autocatalysis by acidic degradation products explains the high rates they saw. Pitrolino’s chitosan study expects the opposite for its material, with higher porosity speeding degradation through more surface, citing earlier chitosan work. Test the porosity you’ll implant rather than a denser or more open stand-in.
For a printed scaffold, the lay-down pattern sets the starting stiffness and how it falls. Ferreira and colleagues printed PCL scaffolds from one filament spacing at three angles. At day 0, compressive modulus was 52.1 MPa for a 0/90° pattern and 16.2 MPa for 0/45/90/135°. In lipase, the 0/90° scaffolds fell steadily to 3.3 MPa by day 20, while the 0/45/90/135° ones dropped to 5.2 MPa at day 15 and read 8.2 MPa at day 20. Weight loss followed the same linear trend whatever the pattern. Print test pieces on the device’s own settings.
Which readouts does a scaffold degradation study need?
A scaffold degradation study needs mass, molecular weight and mechanics at least, because they can move on separate schedules. Mass loss, molecular weight and erosion covers how to run them.
| Readout | What it shows for a scaffold | Standard reference |
|---|---|---|
| Mass loss | How much material has left | ASTM F1635 (mass loss rate) |
| Wet (hydrated) mass | Water uptake and loss on the same sample over time | None in the scopes read |
| Molecular weight | Chains breaking, often before mass falls | ASTM F1635 (molar mass), ISO 13781 (chemical changes) |
| Compressive or tensile properties | Whether the scaffold still carries load | ASTM F1635, ISO 13781 (mechanical changes) |
| Pore structure (SEM, micro-CT) | Whether the architecture holds | None in the scopes read |
| Degradation products in the medium | What leaves the scaffold, and when | ISO 10993-13, for non-resorbable polymers |
In Ferreira’s and Pitrolino’s scaffolds, the readouts parted:
- Molecular weight held while stiffness and mass fell: Ferreira’s PCL scaffolds in lipase lost up to 72.2% of their mass and most of their modulus, with molecular weight almost unchanged, which the authors read as surface erosion.
- Mass fell while stiffness held: Pitrolino’s chitosan scaffolds lost 10 to 16% of their mass by day 28. On the composite scaffold, compressive strength rose slightly by day 3 as it hydrated, from 4 to 6 or 7 kPa, and the authors report that degradation had no statistically detectable effect on strength or modulus over 21 days.
The degradation testing guide covers Agrawal’s PLGA modulus, which rose before it fell. The swelling ratio page covers wet against dry mass.
Can a hotter run stand in for 37 °C?
A hotter run can shorten a long study, and the evidence for it here is narrow. Weir and colleagues degraded ethylene oxide sterilized PLLA tensile specimens at 50 and 70 °C and found a mechanism very similar to that at 37 °C. They still flag the validity of testing above the polymer’s glass transition temperature, and the significance of autocatalysis when hot, as open concerns. That result covers PLLA. For PLGA or a blend, measure its glass transition temperature in the hydrated state before choosing a temperature.
Run a 37 °C arm alongside any hot one until the two agree on the order of your candidates.
Where does in vitro degradation testing stop?
An in vitro test can’t settle how the device behaves in the body. ISO 13781’s scope says its methods can’t definitively predict in vivo behaviour unless validated for the specific device.
ISO 10993-13 covers generating, identifying and quantifying degradation products from polymeric devices, with an accelerated test as a screening method. Its scope considers only non-resorbable polymers, says modified procedures may suit resorbable ones, and leaves out degradation driven by enzymes, cells, mechanical stress or wear. On October 29, 2024, it was marked for revision, and a new edition is in development.
Degradation products can affect cells whatever the mass curve does. Pitrolino measured about 2 mM glucosamine in the medium at days 14 and 21, and in a separate test, 2 mM glucosamine cut mesenchymal stem cell numbers threefold against controls. A mass curve can’t see that, and judging it belongs to biocompatibility testing.
What a GelTech study measures on scaffold and implant degradation
GelTech tests the rods, discs and scaffolds the tissue engineering page lists. Carousel weighs each sample drained and wet, in place, at every timepoint, six samples at a time, from ambient to 60 °C, and its mass data carries roughly 3x less data variability than manual work. That curve sits beside F1635’s mass loss at set timepoints and never replaces it. Molecular weight runs in GelTech’s own lab on separate samples, and stiffness (G′, G″ and compressive modulus) comes from integrated instruments on separate samples.
Size the sample first. Carousel needs at least 25 mg of dry sample and reads to 1 mg. By our arithmetic, 1 mg is 2.5% of a 40 mg scaffold, so a small scaffold’s wet curve gives shape and timing, and the F1635 mass loss figure comes from dry weighing. GelTech doesn’t run animal or clinical studies, or accredited biocompatibility or sterility testing. See what to put in a study brief.
Sources
- ASTM F1635-24, Standard test method for in vitro degradation testing of hydrolytically degradable polymer resins and fabricated forms for surgical implants (public scope and significance)
- ISO 13781:2017, Implants for surgery, homopolymers, copolymers and blends on poly(lactide), in vitro degradation testing (public scope)
- ISO 10993-13:2010, Biological evaluation of medical devices, part 13: identification and quantification of degradation products from polymeric medical devices (public scope and status)
- Holy CE, Cheng C, Davies JE, Shoichet MS. Optimizing the sterilization of PLGA scaffolds for use in tissue engineering. Biomaterials. 2001;22:25-31
- Agrawal CM, McKinney JS, Lanctot D, Athanasiou KA. Effects of fluid flow on the in vitro degradation kinetics of biodegradable scaffolds for tissue engineering. Biomaterials. 2000;21:2443-2452
- Ferreira J, Gloria A, Cometa S, et al. Effect of in vitro enzymatic degradation on 3D printed poly(ε-caprolactone) scaffolds: morphological, chemical and mechanical properties. J Appl Biomater Funct Mater. 2017;15(3):185-195
- Pitrolino K, Felfel R, Roberts G, et al. In vitro degradation of a chitosan-based osteochondral construct points to a transient effect on cellular viability. Biomed Mater. 2024;19:055025
- Weir NA, Buchanan FJ, Orr JF, Farrar DF, Dickson GR. Degradation of poly-L-lactide. Part 2: increased temperature accelerated degradation. Proc Inst Mech Eng H. 2004;218:321-330
Related reading
GelTech services and industries
Questions
Is ethanol disinfection good enough for scaffold degradation samples?
Ethanol disinfection of a PLGA scaffold changed neither its shape nor its molecular weight in a 2001 study, which makes it a useful comparison arm. The same authors say it doesn't reliably kill hydrophilic viruses and bacterial spores, so it doesn't stand in for the sterilization the device will get.
Does a scaffold's porosity stay the same while it degrades?
A scaffold's porosity can change during degradation. In a 2000 PLGA study, porosity fell for the first two weeks and then rose, and in a 2024 chitosan study, mean pore size grew from about 184 to 229 µm in the first three days. Measure porosity at more than one timepoint if the rate depends on it.
How long does a PLLA implant take to resorb?
A PLLA orthopaedic device takes more than five years to resorb fully in a normal physiological environment, according to the background of a 2004 study of accelerated degradation. That timescale is why hotter, accelerated runs get used for PLLA, with their limits stated.