Hydrogel rheology and swelling

In hydrogel rheology, the storage modulus and the swelling ratio read the same crosslink density from two sides: a denser network is stiffer and takes up less fluid. In one PEG hydrogel study, mesh sizes from the two routes differed by 9 to 21% at the ends of two composition series, with the modulus route larger. That modulus route also used the swelling ratio, so some agreement is built in.

Storage modulus rises with crosslink density, and swelling falls with it. Rubber elasticity ties the shear modulus to the network’s density and the molecular weight between crosslinks. In Li and Mooney’s form, mesh size scales with the inverse cube root of the shear modulus. By our arithmetic, a gel eight times stiffer has a mesh about half as wide, since 8 to the power of −1/3 is 0.5.

Swelling reaches the same network through the Flory-Rehner balance, which the hydrogel characterization guide sets out. Rehmann, Kloxin and colleagues used a form of the rubber elasticity equation that includes the polymer volume fraction. They measured the modulus right after the gel formed, at 1% strain and 2 Hz, then corrected it to the swollen state through the cube roots of the swelling ratios. So in their method the modulus-based crosslink density already depends on a swelling measurement.

What is tan delta in hydrogel rheology?

Tan delta is the loss modulus over the storage modulus, G″/G′, and it tells you how solid or liquid the gel behaves at the frequency you tested. In Bercea’s review, a liquid-like sample has tan delta above 1, G′ and G″ cross near 1 at gelation, the value drops “slightly below 1 for networks with very low crosslinking degree”, and it keeps falling as the structure forms. Most hydrogels in the literature sit around 0.1 and form very stiff networks, the review says, and it cites a study that put gelatin methacrylamide, gellan gum and methyl cellulose gels between 0.01 and 0.1.

Tan delta is a ratio, so it says nothing about stiffness on its own. Two gels can share a tan delta of 0.1 with moduli a decade apart. Read it beside G′.

Frequency matters too. Sun Han Chang and colleagues describe the Winter gel point as the moment G′ and G″ follow the same power law in frequency. By our arithmetic, two moduli on the same power law have a constant ratio, so tan delta is the same at every frequency at the gel point. That constant depends on the power-law exponent, so it equals 1 only for one exponent, and the crossover where tan delta reads 1 is an approximation. The authors add that fast-gelling systems change too quickly to measure G′ and G″ across frequencies, which is why the crossover gets used instead.

How do you test a swollen hydrogel on a rheometer?

Test a swollen gel after it has reached equilibrium in its medium, held by enough normal force to stop slip, kept wet, and inside its linear range. Baker and colleagues give a worked protocol for polyacrylamide discs about 1 mm high.

  • Equilibrate: they swelled discs for 24 hours in isotonic solution and blotted the excess before loading. A gel tested as made and one tested swollen give two different moduli.
  • Gap and normal force: they lowered a 25 mm plate until the axial force read 0.01 to 0.2 N. The swollen disc’s height sets the gap, and the force that holds it also compresses it.
  • Slip: they used sandpaper on one formulation and a bare plate on the other, and excluded any sample that slipped.
  • Sweeps first: Baker ran a stress sweep first, to find the stress giving 1% strain, then frequency sweeps below that stress, and reported data only to 10 Hz, because “inertial forces dominate the data beyond that”. Chen, Burdick and colleagues ran a frequency sweep at 0.2% strain before their strain sweep, so the order varies; either way, the frequency sweep belongs inside the linear range.
  • Dehydration: Baker’s paper describes no evaporation control. Chen and colleagues list “Hydrogel dries out during testing” as a known problem, and ring the solvent trap with water to keep the gel hydrated.

Weighing the disc before and after the run shows whether it lost water on the plate. That check is our suggestion rather than a step from these papers.

Why do rheology and swelling disagree?

They disagree when they measure different states, carry different errors or rest on different assumptions. Rehmann and colleagues found the two “give relatively consistent results” for the step-growth PEG gels they tested, with rubber elasticity giving slightly larger mesh sizes. Five things separate the two readouts.

  • Different states: the modulus came from the gel as made and the swelling from the gel at equilibrium, joined by a correction that uses the swelling ratio.
  • Stacked error: “rubber elasticity incorporates experimental error from both modulus and swelling measurements”, the authors write, so swelling alone is “more precise (but not necessarily more accurate)”.
  • Different sensitivity: changing the crosslinker shifted mesh size by swelling (p < 0.05) and not by rubber elasticity (p = 0.41).
  • Model assumptions: both routes were built on synthetic networks, and the hydrogel characterization guide notes that gelatin methacrylamide gels didn’t follow the same swelling relationships.
  • The medium and the clock: swelling moves with ionic strength and pH, as the hydrogel swelling ratio page shows, and both readouts move as a gel degrades. A modulus from day one and a swelling ratio from day seven describe two gels.
Rheology readout What it means for a hydrogel What swelling adds
G′ in the linear range Stiffness, and through rubber elasticity a crosslink density A second crosslink density estimate, and the volume fraction that some forms of the modulus route need
G″ Energy lost per cycle No direct counterpart; read it through tan delta
Tan delta How solid the gel behaves at that frequency How much fluid the network holds at that stiffness
G′ and G″ against frequency Whether the network is formed, and the gel point Whether the formed gel keeps taking up fluid afterward
G′ after days in medium How the network changes with time The swelling curve over the same days, which shows whether softening tracks uptake

To take that swelling curve without lifting the gel, see automated hydrogel swelling measurement. Rheology for injection sits in injectable hydrogels for drug delivery.

What a GelTech study measures on rheology and swelling

Rheometry is among GelTech’s integrated instruments, and the rheology and mechanical service lists G′ and G″, tan δ, viscosity, modulus and frequency sweeps. Carousel records the swelling side: drained wet mass to 1 mg at every timepoint, in a 24 mL sample chamber inside a 50 mL incubation chamber, six samples at a time, for weeks to months. Carousel’s mass data carries roughly 3x less data variability than manual work. Stiffness, as G′, G″ and compressive modulus, comes from separate samples at set timepoints, measured on integrated instruments and read beside Carousel’s mass curve.

GelTech doesn’t run animal or clinical studies, or accredited biocompatibility or sterility testing. See R&D services and how a pilot study works.

Sources

Related reading

GelTech services and industries

Questions

What tan delta value means a hydrogel has fully formed?

No single tan delta value marks a fully formed hydrogel. The value keeps falling as the network builds, so compare formulations at the same frequency, strain and time after mixing, and watch for G′ to level off.

Should a hydrogel be tested on the rheometer as made or after swelling?

A hydrogel can be tested as made or after swelling, and the two give different moduli, so report which state you tested. Rehmann and colleagues tested as made and corrected to the swollen state; Baker and colleagues swelled their discs for 24 hours before testing.

Can rheology replace a swelling test?

Rheology can't replace a swelling test, because the modulus gives a crosslink density estimate without showing how much fluid the gel takes up, how fast, or how the medium changes that. Swelling is also the cheaper readout to repeat over weeks.

A row of palm trees against a blue sky

Need a material characterized?

Send your formulation and plan the study with the team.

By sending, you agree to our terms and privacy policy. Please leave out confidential formulation details until an NDA is in place.